Teknos tuotteet

Teknoksen offline-tuotetietokirjasto

  • Jälleenmyyjien käyttöön sävytyskoneille Teknoksen tuotetiedot helppokäyttöisessä muodossa.

NORDICA MATT House Paint

      

Full-matt water-borne acrylate-based paint for wooden surfaces outdoors. NORDICA MATT has a matt and hard surface that is dirt-repellent and retains its appearance and colour for a very long time.

For new and previously with acrylate- and oil paint painted wooden surfaces and for industrially primed and/or undercoated wooden surfaces, e.g. exterior walls, facial boards and weather boards.

Technical Data

Solids

About 36 % by volume

Volatile organic compound (VOC)

EU VOC limit value (kat A/d): 130 g/l. The product's VOC: max. 130 g/l.

Practical spreading rate

5 - 8 m²/l

Density

1.2 g/ml

Drying time at +23 °C / 50 % RH

- touch dry

- overcoatable

after 1 hour

after 4 hours

The drying process will be slower in cold and/or damp.

Thinner, clean up

Water. Wash the equipment immediately after use with detergent and warm water.

Finish

Full-matt

Colours

Base 1 (white), base 3, base 5 (red) and black standard colour

The paint is included in the Teknomix tinting system.

Weather resistance

Very good.

Packages (availability varies by country)

Base paints 1 and 3: 0,45 L, 0,9 L, 2,7 L, 9 L, 18 L

Base paint 5: 0,9 L, 2,7 L, 9 L, 18 L

Standard colour: 0,9 L, 2,7 L, 9 L

SAFETY MARKINGS

See Safety Data Sheet.

Direction for Use

Surface preparation

NEW WOODEN SURFACE:

Treat the surface as soon as possible. At least the impregnation and priming would be best done in the summer of construction.

Remove from the surface all loose matter, dirt, dust and mildew. If needed, use RENSA FACADE facade cleaner.

PREVIOUSLY PAINTED OR OLD WOODEN SURFACE:

Replace wooden parts that are in poor condition. Remove loose matter, dirt and dust. Remove loose and poorly adherent old paint. Wash the surface with RENSA FACADE facade cleaner.

Remove the deteriorated paint coats carefully. The adherence of an old thick paint layer to the substrate may have been weakened, therefore the paint should be removed completely although the paint film looks intact. The old paint layer is removed by scraping, by wire brushing or by burning off (e.g. by warm-air heater or infrared heater). Secondarily paint remover or blasting can be used.

Clean rusty steel parts: by sanding, wire brushing eg.

Priming

Bare wooden surface is primed with clear WOODEX AQUA BASE priming oil. If the wooden surface is old and primed with oil or painted with oil paint, solvent-borne WOODEX BASE priming oil is used.

Priming

The surface treated with priming oil is then primed with NORDICA PRIMER. If the surface is an old wooden surface primed with oil or painted with oil paint, use solvent-borne PUUPOHJA alkyd primer diluted 10-15 % by volume.

Rusting steel surfaces are primed with FERREX AQUA anticorrosive paint.

Also the end grains of industrially primed and/or undercoated timber needs to be treated with priming oil or primed before applying top coat.

Top coating

Before use stir the paint thoroughly. Dilute the paint 5 - 10 % by volume by water, when required.

Reserve a sufficient amount of paint in the same vessel for each uniform surface. Colour differences will thus be avoided.

Apply the paint by brush. If the paint is applied by airless spray, the surface is to be finished by a brush. Recommended airless spray nozzle is 0.015 - 0.019".

Application conditions

The surface to be painted has to be dry. The moisture of the wood must be below 20 % of the dry weight of the wood. During the application and drying period (also the following night after the painting work needs to be taken into account), the temperature of the ambient air, the surface and the paint shall be above +5 °C and the relative air humidity below 80 %.

Storage

Must not freeze.

The information of this data sheet is based on laboratory tests and practical experience. The figures are for guidance only and depend on, for example, colour and gloss. As we have no control over the use and application conditions, we are only responsible for the quality of the product and guarantee that it conforms to our quality control. We accept no liability for any loss or damage resulting from the application of the product contrary to the directions or the intended use. The latest versions of our data sheets, material safety data sheets and system sheets are on our home pages www.teknos.com.